A2 Ball Clay

A2 Ball Clay

Description

A smooth and highly plastic, buff burning, refractory, coarse grained, lignitic ball clay. A2 is mined in Southern Saskatchewn and is both a ball clay and a fireclay. We have large reserves of this material. Ball clays are suitable in a wide range of ceramic and non-ceramic applications. When A2 is fine ground and impurities air-separated (which we do not currently do) it is very similar to commercial ball clays from the southern USA (although darker burning).

While kaolin is white and clean and considered pure clay mineral, ball clays, by comparison, are generally grey or brownish in color and differ in the following ways:

The principal properties of ball clays that make them most useful in ceramics are:

A2 being mined at Plainsman quarry in southern Saskatchewan

Process Properties

As a ball clay, it improves the plasticity of any body recipe to which it is added. However, it will also increase drying shrinkage, slow down drying time and increase the difficulty of drying ware without cracking.

A2 contains some soluble salts. These are hostile to the deflocculation process - so this material is not suitable in casting body recipes.

Although A2 powder looks like many other ball clays, it is not fine-ground to 42 mesh (we do not have equipment for 200 mesh). A2, as supplied by us, is not suitable in porcelains or whitewares. However, in native rustic stonewares it contributes and earthy and natural look to the fired surface.

Other applications: We can produce custom lesser mesh sizes and package in bulk bags for non-ceramic applications (please call).


A2 stockpiles at the quarry (in various states of weathering).

Firing


A2 42 mesh at cone 10R

A2 has significant iron content so it does not fire white. The soluble salts in A2 will produce a flashing effect during firing in reduction, turning the cream colored surface to brownish. Since we only grind the standard material to 42 mesh, A2 will bring fired speckle to reduction bodies (these are ironstone concretion particles that fuse in reduction atmospheres).


A2 fired bars (cone 10R top) and cone 11 oxidation. Ground to 10 mesh. Formerly called PlasticFire.

Physical Properties

 Drying Shrinkage (50:50 calcine:raw mix): 5.5-6.5%
 Drying Factor (50:50 calcine:raw mix): C130
 Dry Density (50:50 calcine:raw mix): 1.80

Sieve Analysis (Tyler mesh):

   35-48: 0.1-0.4%
   48-65: 1.0-3.5
  65-100: 1.5-5.5
 100-150: 1.0-4.0
 150-200: 3.0-7.0
 200-325: 5.0-9.0

Fired Shrinkage (50:50 calcine:raw mix):

  Cone 6: 4.0-5.0%
  Cone 8: 4.5-5.5
 Cone 10: 5.5-6.5
 Cone 11: 5.5-6.5

Fired Absorption: (50:50 calcine:raw mix)

  Cone 6: 11.0-15.0%
  Cone 8: 9.0-11.0
 Cone 10: 7.0-9.0
 Cone 11: 6.0-8.0

Chemical Analysis

 CaO      0.25
 K2O      0.69
 MgO      0.43
 Na2O     0.04
 TiO2     0.72
 Al2O3   18.99
 SiO2    65.12
 Fe2O3    1.84
 LOI     10.58%