F100G

Description

White grogged sculpture body made from talc and ball clay (the same recipe as L213 but 20% of the talc has been substituted for 35 mesh grog and silica sand). This body is commonly used to make large pieces.

News

We no longer produce this but you can make your own by wedging in sand and/or grog to our Snow body. An advantage of this approach is better glaze fit than was afforded by F100G.

Process Properties

Talc/Ball clay bodies are very plastic and at the same time dry well. The additional fine silica sand and grog give this body even better drying capabilities. Despite this, F100G feels quite smooth. We recommend F100G when sculptors need high certainty that ware can be dried without cracks while still having a relatively smooth fired surface. One caution: Its dry strength is fairly low, handle dry ware with care.


Closeup on the thrown surface of F100G. Although grogged, it is much smoother than a typical sculpture body.

Firing

Very white burning. The high plasticity of F100G slows drying and makes it susceptible to failure in the early water-smoking phase of firing. Make sure pieces are thoroughly dry before firing. Preheat your kiln overnight, or even for a full day, if pieces are large.

F100G can be fired to cone 4 fairly safely. At cone 6 it still appears to be stable visually, however the fired shrinkage and porosity have already reversed (indicating firing volatility).


F100G fired to cone 04, 02, 2, 4, 6 (bottom to top). Notice the color changes to yellow at cone 6.

Glazing

Most customers use this as a sculpture body, they do not glaze pieces. Although we have had some success with the G2931K base glaze, like F100, we do not have any specific glaze recipe recommendations - you will need to experiment to find one available to you that fits.


F100G with Zero3 K glaze and fired to cone 03.

Thermal Expansion

We do not supply thermal expansion values. If a chart is supplied here, please view it only as a way to compare one body with another. Please note that, although you may calculate the thermal expansion of a glaze, this cannot be done for clay bodies since they do not melt. The best way to fit glazes to clay bodies is by testing, evaluation, adjustment and retesting. For example, if a glaze crazes, adjust its recipe to bring the expansion down, fire a glazed piece and thermal stress it (using an IWCT test, 300F into ice-water). If it still crazes, repeat the process.

Physical Properties

 Drying Shrinkage: 4.5-5.5%
 Dry Strength: n/a
 Drying Factor: B110
 Water Content: 19.5-20.5% Mar 99
 Dry Density: 1.95

Sieve Analysis (Tyler mesh):

     +48     (300 microns): 0.0-0.6%
   48-65 (300-210 microns): 0.4-0.8
  65-100 (210-149 microns): 2.5-3.5
 100-150 (149-106 microns): 2.0-3.0
 150-200  (106-75 microns): 5.5-7.5
 200-325   (75-45 microns): 7.0-10.0

Fired Shrinkage:

   Cone 04: 1.0-2.0%
  Cone 02: 1.5-2.5
  Cone 2: 2.0-3.0
  Cone 4: 2.5-3.5
  Cone 6: 2.0-3.0
 

Fired Absorption:

   Cone 04: 11-14%
  Cone 02: 10.5-13
  Cone 2: 10-12
  Cone 4: 10-11.5
  Cone 6: 9.5-11

Gallery


F100G sculpture by Mary Stankevicius


This incredible house was made by Kira Vlietstra, a first-year visual communications student at our local college. It is 18" high, her first attempt, a testimony to how well this clay works for hand building.


F100G dragon by Mary Stankevicius


F100G Boars by Mary Stankevicius

Logo Plainsman Clays
671 Industrial Ave. SE, Medicine Hat, Alberta T1A 3L5
Phone: 403-527-8535 FAX:403-527-7508
Email: tim.lerner@plainsmanclays.com