Sandy brown stoneware. This is a mixture of two light-duty fireclays (20% IMCO M-4, 20% IMCO 400), OM#4 ball clay (20%), IMCO Burgundy low fire red burning clay (20%), 15% silica sand and 4% Mulcoa 47-35 grog.
In 2016 the red clay/flux portion of the recipe, "Banta Red", was no longer available. The supplier, IMCO, recommended their Burgundy clay as a substitute, we tested that and began using it instead. It was not as strong a flux, so some density was compromised, increasing the body porosity. But it was not enough to be an issue. But F95 has become even less vitreous (meaning further loss of maturity in one-or-more of the IMCO 400, IMCO M-4 and/or Burgundy ingredients). We have found a solution that greatly improves the density of current runs: An 85:15 mix of F95 and L210 moves porosity down to about 4%. You can even adjust the proportion to suit (e.g. a 75:25 mix will deliver 2.7% porosity at cone 6 but the color will darken somewhat). This blend actually improves body workability also, making it more plastic.
F95 is light-green-colored in the wet state. The 60% fire clay/ball clay content means that is easy-to-throw, even when quite soft. Although it contains grog and sand, it feels smooth to throw without generating excessive slip during throwing (of course it is somewhat abrasive against the wheelhead).
The leather-color of F95 at cone 6 depends on it NOT being vitreous (if fired to oxidation maturity, beyond cone 8, surface aethetic is lost as it turns solid greenish). Fired porosity at cone 6 is intended at 5% (a typical stoneware is half of that).
Because this body contains significant percentage of silica sand it is subject to cracking if ware is fired up or down through quartz inversion temperature too fast. The grog and silica sand also increase the fired porosity. The sand and grog are needed to cut the drying shrinkage in this otherwise very plastic blend of clays.
The centre bar, and one below it, are fired to cone 5 and 6, they are burning the intended light sandy tan. By cone 8, the top bar, the color is lost as vitrification begins (these bars were made in 2010 when Banta was still available).
Because F95 does not fire vitreous at cone 6, glazes must fit (not craze) to avoid seepage of water. If you need help to deal with a crazing issue please contact us. To guarantee the clay will not seep please use a higher percentage of L210 (as noted above).
To mix this body yourself you could simply use 60% ball clay and 20% Redart as a starting point (with sand and grog). Redart, a low fire and consistent red-burning body, is available everywhere. IMCO 400 and M-4 are similar to Lincoln Fireclay, if you can get that then use 40% Lincoln and 20% ball clay). Experiment with different proportions of Redart to achieve the compromise of color and maturity desired (remembering that you will have to settle for non-vitreous to achieve this type of color).
We do not supply thermal expansion values. If a chart is supplied here, please view it only as a way to compare one body with another. Please note that, although you may calculate the thermal expansion of a glaze, this cannot be done for clay bodies since they do not melt. The best way to fit glazes to clay bodies is by testing, evaluation, adjustment and retesting. For example, if a glaze crazes, adjust its recipe to bring the expansion down, fire a glazed piece and thermal stress it (using an IWCT test, 300F into ice-water). If it still crazes, repeat the process.
Drying Shrinkage: 5.5-6.5% Drying Factor: C120
Cone 4: 4.0-5.0% Cone 6: 4.5-5.5 Cone 8: 5.0-6.0
Cone 4: 5.5-7.0% Cone 6: 4.0-5.0 Cone 8: 2.5-3.5
![]() |
Plainsman Clays 671 Industrial Ave. SE, Medicine Hat, Alberta T1A 3L5 Phone: 403-527-8535 FAX:403-527-7508 Email: tim.lerner@plainsmanclays.com |