Cone 6 Alberta Slip Glazes
This is not a glaze recipe page. Alberta Slip is a glaze material, these are demonstration recipes of what can be done with it.
These are "not guaranteed-to-work glazes". This page focusses on the value of this material to make base glazes and provides some examples of variations. However circumstances differ, do testing and alter for your situation (for information on variegating, opacifying and coloring glazes click here). Care should be taken not to fire glazes too fast or at too low of a temperature. Witness cones are recommended to assure you have reached cone 6. These glazes have worked in our studio at Plainsman Clays but we recommend testing them in your circumstances and on your clay bodies for fit. For functional glaze, consider testing for leaching, crazing and cutlery marking. Courtesy of Digitalfire Reference LibraryAlberta Slip Cone 6 Black Code: GA6-H Pure Alberta Slip can be made into a black adding only 20% frit and 3% black stain
The firing schedule may be important to developing this glaze effect. A glossy black. The small amount of frit needed is due to the fact that Alberta slip is a dark burning material already. If it is not black enough, increase the percentage of stain. If you need a glossier surface, increase the frit. If it crazes switch to Ferro Frit 3195. Should be ball milled. ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram.
Alberta Slip Cone 6 Oatmeal Code: GA6-F Plainsman Cone 6 Alberta Slip based glaze. It can be found among others at http://albertaslip.com.
The firing schedule may be important to developing this glaze effect. Alberta slip is well suited to oatmeal glazes because it already has the iron content needed. Vary the titanium for more or less variegation and oatmeal appearance. ![]() How much rutile can a glaze take before it becomes unstable? The 80:20 base GA6-A Alberta slip base becomes oatmeal when over saturated with rutile or titanium (left: 6% rutile, 3% titanium; right: 4% rutile, 2% titanium). That oatmeal effect is actually the excess titanium crystallizing out of solution into the melt as the kiln cools. Although the visual effects can be interesting, the micro-crystalline surface is unpleasant to touch and susceptible to cutlery marking and leaching (not as stable or durable as in glazes which are pure amorphous glass). For functional ware, rutile glazes are among the most troublesome to keep consistent, one way of avoiding problems is keeping the percentage as low as possible while still getting the desired variegation (of course that will vary depending on the melt fluidity of the glaze, more highly fluid ones can handle more rutile or titanium). ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram.
Alberta Slip Cone 6 transparent honey glaze Code: GA6-A An amber-colored glaze that produces a clean, micro bubble free transparent glass on brown and red burning stonewares.
The firing schedule may be important to developing this glaze effect. This is the base cone 6 Alberta Slip recipe. The 20% frit makes it melt well to form a transparent amber glossy. ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram. ![]() Alberta Slip GA6-B base darkened with iron oxide Fired to cone 6 using the C6DHSC schedule. Top: GA6-B. This recipe is 80% Alberta slip and 20% Ferro Frit 3195 (we used to use frit 3134 but have found frit 3195 works much better). Bottom: We added 1, 2, 3 and 4% iron oxide. At about 2%, the color matches the rich reddish effect you would get if you used an 80:20 Albany:3195 recipe (without an iron addition). An added benefit is that the iron acts as a fining agent to remove micro-bubbles to achieve better transparency. ![]() A cone 6 clear glaze plus iron vs. Alberta Slip amber base These two mugs are made from a dark red burning stoneware and fired in a cool-and-soak firing schedule. A white engobe (L3954A) has been applied on the inside and half way down the outside. Both are glazed inside with G2926B whiteware transparent glaze. The outside glaze on the left is the same transparent with 4% added iron oxide. It has been sieved to 80 mesh. Notice the iron agglomerates and still produces specking (an effect that may be desired, but difficult to keep consistent). Interestingly, that iron is producing a clear amber-colored glass about equal in color to the Alberta Slip GA6A base glaze (80% Alberta Slip, 20% Frit 3195) on the mug on the right. Neither has the micro bubbles that mar a typical clear glaze on bodies like this. ![]() A transparent that looks good on cone 6 red burning bodies The GA6-A Alberta Slip:Frit 3134 (80%:20%) glaze is excellent as a liner for dark burning bodies, it looks much better than a regular transparent recipe (which often form clouds of bubbles on red bodies). The iron in this glaze makes it fire an amber color on buff burning bodies (not very attractive), but on red bodies it brings out the natural color of the clay. ![]() Plainsman dark bodies with Alberta Slip floating blue Cone 6 mugs made from Plainsman M350 (left) and M390 dark burning cone 6 bodies. The outside glaze is Alberta-Slip-based GA6-C rutile blue and the inside is GA6-A base (20% frit 3134 and 80% Alberta Slip). That inside glaze is normally glossy transparent amber, but crystallizes to a stunning silky matte when fired using the C6DHSC schedule. ![]() A typical transparent glaze vs. Alberta Slip amber base on a red burning cone 6 body The body is Plainsman M332, a coarse particled brown to red burning cone 6 body. With the G2926B transparent cone 6 glaze (left) and the GA6-A Alberta Slip base (right). The latter brings out the color of the body much better, the former is milky, bubbly and yucky! ![]() GA6A Alberta Slip base using Frit 3249 and 3195 on buff body The body is buff burning Plainsman M340 (cone 6). The amber colored glaze is 80% Alberta Slip (raw:calcine mix) with 20% of each frit. The white engobe on the inside of mug 1 is L3954A (also glazed inside using transparent G2926B). These frits are producing an amber gloss glaze of high quality. On the outside of mug 1 we see the 3195 version on the white slip until midway down, then on the bare buff clay (the other has the 3249 version). These mugs are fired using a drop-and-soak firing schedule. A couple of caveats: Frit 3249 has a very low thermal expansion, use it on bodies that craze other glazes (like Plainsman P300), it could shiver on stonewares like this. Both of these frits prevent the formation of bloating blues (with additions of rutile or titanium). ![]() A white engobe on dark and buff burning cone 6 stonewares Left is Plainsman M340. Right is M390. Each mug has been white-engobed inside (by pouring), using L3954B, and halfway down the outside (by dipping). The insides have been glazed using G2926B clear. The inside surface has more depth and a richer appearance than could be achieved using a white glaze (especially over the dark burning body). The outside of the left one is Alberta Slip base GA6-B. The outside glaze on the right is the clear plus 4% iron oxide. This technique of using the engobe enables porcelain-like functional surfaces on the insides and the visual contrasts and character on the outsides of the stoneware mugs. ![]() Crystallization of this glaze gives insight into why it can host the floating blue effect These two mugs have the Alberta Slip base cone 6 GA6-A glaze on the inside and GA6-C on the outside (it just adds rutile to GA6-A). The left one was cooled normally (kiln off at cone 6 after soak). For the mug on the right, the kiln was soaked for half an hour at 1800F on the way down to develop the rutile blue glaze on the outside. But during this period crystallization occurred on the inside also. This provides an insight into my this GA6-A base hosts floating blue effects but GA6-B does not: The amount of Al2O3 is much lower, that improves melt fluidity and acts as a catalyst for crystallization. ![]() Same glaze, same kiln, same clay: The right one crystallized. Why? Well, actually they are not exactly the same. This is 80% Alberta Slip and 20% frit. But the frit on the left is Ferro 3195 and on the right is 3134. By comparing the calculated chemistry for these two we can say that the likely reason for the difference is the Al2O3 content. Frit 3134 has almost none whereas 3195 has 12%. Al2O3 stiffens the glaze melt, that impedes crystal growth. And it stabilizes the melt against running during firing. Frit 3195 is thus much more "like a glaze" than is 3134, it is what Alberta Slip needs to melt as a transparent glass under normally cooling in the kiln. ![]() GA6A Alberta Slip base using Frit 3124, 3249 and 3195 on dark body The body is dark brown burning Plainsman M390 (cone 6). The amber colored glaze is 80% Alberta Slip (raw:calcine mix) with 20% of each frit. The white engobe, L3954B, on the inside of two of the mugs is L3954A (those mugs are glazed inside using transparent G2926B). The Alberta Slip amber gloss glaze produces an ultra-gloss surface of high quality on mugs 2 and 3 (Frit 3249 and 3195). On the outside we see it this glaze on the white slip until midway down, then on the bare red clay. The amber glaze on the first mug (with Frit 3124) has a pebbly surface. These are fired using a drop-and-soak firing schedule. Some caution is required with the 3249 version, it has low thermal expansion (that is good on bodies that normally craze glazes, but risks shivering on ones that do not).
Alberta Slip Floating Blue Cone 6 Code: GA6-C Plainsman Cone 6 Alberta Slip based glaze the fires bright blue but with zero cobalt.
The firing schedule may be important to developing this glaze effect. This glaze creates a rich blue yet contains none of the world's most expensive common ceramic material, cobalt oxide. On dark bodies the depth of color is incredible. It has a great glossy surface, and, because it contains no raw metal oxides or stains, toxicity issues are less of a concern. On lighter bodies it variegates from medium steel blue, where it is very thick, to amber clear (or a brown if the body is dark) where thin. The blue color does not develop well on porcelains or white-burning stonewares (unless you underlay it with a dark-colored engobe). This glaze requires a slow-cool firing schedule to work (see the paragraph below). ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram. ![]() GA6-C on a light and dark burning clay body at cone 6 Left: Plainsman 3D, a raw quarry material that fires as a buff stoneware at cone 6-8. Right: Plainsman Coffee clay (stained black using raw umber). Both were fired using the C6DHSC firing schedule. The inside glaze is the GA6-B Alberta Slip base. As of Dec/2021 cobalt retails at $100/500g! Yet the deep blue color on the mug on the right contains zero cobalt, the color is from titanium and iron. This GA6-C blue happens with any dark burning body, or with light burning ones having a dark engobe (e.g. L3954B with a dark colored stain) under the glaze. ![]() Ravencrag Slip vs Alberta Slip floating blues at cone 6 oxidation Usable, reliable, non-crazing floating blue glazes are difficult to achieve at cone 6. Not these, they pass all the tests yet fire like the original classic G2826R floating blue from David Shaner. Both have been applied at moderate thickness on Plainsman M325 (using a slurry of about 1.43-1.45 specific gravity, higher values end up getting them on too thick). The GR6-M Ravenscrag version (left) highlights contours better (the edges are black because of the black engobe underneath). It also produces the blue color whether or not the kiln is slow-cooled (although drop-and-hold PLC6DS schedule usually fires more blue). The GA6-C Alberta Slip version has zero cobalt so it is less expensive to make (but it does require the C6DHSC slow-cool firing schedule). It produces a deeper color over the L3954F black engobe on these pieces. Both of these produce a wide range of effects with different thicknesses, bodies and firing schedules. ![]() Alberta Slip rutile blue on a porcelain at cone 6 The glaze recipe is GA6-C. The firing schedule is C6DHSC. The black engobe (applied inside and halfway down the outside) is L3954B. The clay body is Plainsman M370. This demonstrates how different this glaze fires on a white porcelain (bottom half outside) and a black porcelain (the engobed top half). ![]() Plainsman dark bodies with Alberta Slip floating blue Cone 6 mugs made from Plainsman M350 (left) and M390 dark burning cone 6 bodies. The outside glaze is Alberta-Slip-based GA6-C rutile blue and the inside is GA6-A base (20% frit 3134 and 80% Alberta Slip). That inside glaze is normally glossy transparent amber, but crystallizes to a stunning silky matte when fired using the C6DHSC schedule. ![]() Deep, deep blue without any cobalt. How? These have to be seen to be believed, it is the deepest, richest blue we have ever produced. This is Plainsman M340 fired to cone 6. Black-firing L3954B engobe (having 10% Burnt (not raw) Umber instead of the normal 10% Zircopax) was applied inside and partway down the outsides (at the stiff leather hard stage). The incising was done after the engobe dried enough to be able to handle the piece. The glaze is Alberta Slip rutile blue. Firing schedule: Cone 6 drop-and-soak. ![]() Close-up of Floating Blue on cone 6 dark/buff burning bodies This glaze recipe was originally popularized by James Chappell in the book "The Potter's Complete Book of Clay and Glazes", our code number is G2826R. It is and was loved and hated. Why? The high Gerstley Borate content makes it finicky. But the magic ingredient is not the GB, it is the rutile, Rutile makes the cobalt and iron dance. This recipe produces a number of different mechanisms of variegation. Color and opacity vary with thickness. Small rivulets of more fluid glass flow around more viscous phases producing micro-areas of differing colors and opacities. Titanium crystals sparkle and calcium-borate creates opalescence. Bubbles of escaping gases (from GB) have created pooling. Small black speckles from unground or agglomerated particles of iron are also present. Surprise! This is actually GR6-M Ravenscrag Floating blue. All the visuals, but without of the gelling and crazing headaches. ![]() Adding spodumene to this floating blue tones down the white patches GA6-C (left) and GA6-E (right) at cone 6 oxidation. The E version adds 4% spodumene onto the 4% rutile in the C (the base is 80% Alberta Slip and 20% frit 3134). The spodumene eliminate the overly whitish areas that can appear. This glaze requires the "Slow Cool (Reactive Glazes)" firing schedule. It looks the best on dark bodies. ![]() Alberta Slip Rutile blue glaze too thin on a dark body This mug has thin walls and was bisque fired to cone 04 (so it had a fairly porosity). As a result the glaze went on thinner when it was dipped. This was not evident at the time of glazing but at firing the thinner sections produced the brown areas. ![]() GA6-C Alberta Slip rutile blue at cone 5R On Plainsman P300 (left) and M350 (right). The blue effect is darker and richer than oxidation. The richer effect is also partly because the reduction kiln cools slower. ![]() The rutile mechanism in glazes 2, 3, 4, 5% rutile added to an 80:20 mix of Alberta Slip:Frit 3134 at cone 6. This variegating mechanism of rutile is well-known among potters. Rutile can be added to many glazes to variegate existing color and opacification. If more rutile is added the surface turns an ugly yellow in a mass of titanium crystals. ![]() Tin oxide can stop the rutile variegation effect dead in its tracks! This is Alberta Slip (GA6C) on the left. Added frit is melting the Alberta Slip clay to it flows well at cone 6 and added rutile is creating the blue variegated effect (in the absence of expensive cobalt). However GA6D (right) is the same glaze with added Tin Oxide. The tin completely immobilizes the rutile blue effect, it brings out the color of the iron (from the rutile and the body).
Alberta Slip Glossy Brown Cone 6 Code: GA6-D Plainsman Cone 6 Alberta Slip based glaze. It can be found among others at http://albertaslip.com.
The firing schedule may be important to developing this glaze effect. Works well on all types of bodies, very reliable. ![]() Tin oxide can stop the rutile variegation effect dead in its tracks! This is Alberta Slip (GA6C) on the left. Added frit is melting the Alberta Slip clay to it flows well at cone 6 and added rutile is creating the blue variegated effect (in the absence of expensive cobalt). However GA6D (right) is the same glaze with added Tin Oxide. The tin completely immobilizes the rutile blue effect, it brings out the color of the iron (from the rutile and the body). ![]() Variegating effect of sprayed-on layer of titanium dioxide The base glaze (inside and out) is GA6-D Alberta Slip glaze fired at cone 6 on a buff stoneware. However, on the outside, the dried-on glaze was over-sprayed with a very thin layer of titanium and water (VeeGum can be used to help gel the sprayable titanium slurry and suspend it). The dramatic effect is a real testament to the variegating power of TiO2. An advantage of this technique is the source: Titanium dioxide. It is a more consistent source of TiO2 than the often-troublesome rutile. Another advantage is that the variegation can be selectively applied in specific areas or as a design. This effect should work on most glossy glazes having adequate melt fluidity. ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram.
Alberta Slip Lithium Brown Cone 6 Code: GA6-G Plainsman Cone 6 Alberta Slip based glaze.
The firing schedule may be important to developing this glaze effect. One of the most popular Albany Slip glazes was 11% lithium, 4% tin oxide and 85% Albany Slip. This recipe reduces the lithium by more 50% eliminating the shivering problems that were common. This also employs a frit to help melt the glaze (in the absence of the 6% lithium carbonate). The added alumina darkens the color and slightly dulls the gloss (leave it out if you want). ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram. ![]() Alberta Slip used in the common lithium-tin cone 6 glaze This is 85% Alberta Slip, 11% lithium and 4% tin fired at cone 6 in oxidation. Like the original Albany version, it has a very low thermal expansion (because of the high lithium content) and likes to shiver on many clay bodies. ![]() A variation of Albany lithium brown glaze Alberta Slip 75, lithium carbonate 10, tin oxide 4, nepheline syenite 11, calcined alumina 5. ![]() A classic Albany glaze that often shivers These mugs have experienced very serious shivering. This is an Albany Slip glaze with 10% lithium carbonate, it is known to have a very low thermal expansion. This problem can be solved by reducing the amount of lithium or adding high-expansion sodium or potassium. However these fixes will likely affect the appearance. ![]() Adding 6% lithium carbonate to an Alberta Slip glaze does this Left is G3933A, it is an 80:20 mix of our matte and glossy cone 6 base recipes (plus a mix of iron oxide, tin oxide and rutile). The body is Plainsman Coffee Clay. Because of repeated issues with crawling a project was started to create the same effect using Alberta Slip to supply as much of the chemistry as possible. Along that road, the opportunity arose to add lithium (to duplicate Amaco PC-32, a classic Albany/Lithium recipe). That is the glaze on the mug on the right, G3933G1, it has 6% lithium carbonate. Lithium is a super powerful melter, turning this into a very reactive glaze! To make a 500ml jar of brushing glaze, in 2023, required about $7 worth of lithium carbonate.
Alberta Slip Lithium Brown Cone 6 Low Expansion Code: GA6-G1 Plainsman Cone 6 Alberta Slip based glaze. It can be found among others at http://albertaslip.com.
The firing schedule may be important to developing this glaze effect. The regular Alberta Slip lithium brown recipe crazes on porcelain. This one was formulated to maintain the appearance but reduce the thermal expansion. It does this by reducing the KNaO and increasing the MgO. This was effected by employing MgO sourcing frit 3249. This frit is more expensive and difficult to get but it is the only way we have found to effectively reduce the thermal expansion and maintain the aesthetic. ![]() Fine tuning glaze shrinkage vs. hardness These mugs are fired at cone 6 with GA6-G1 Alberta Slip lithium brown. The difference: the ratio of raw to calcine Alberta Slip. In this glaze, a 50:50 ratio was not working well (left). The glaze was shrinking too much on drying, then crawling on firing (it needs to be thickly applied to get the visual effect I want). I mixed the recipe using pure calcine Alberta Slip, then repeated a cycle of pouring a little of this into the 50:50 mix and trying it. I kept doing that and glazing another mug until I had a minimum of drying cracks (while still having good gelling, application properties and dry hardness). The mug on the right was the last cycle, it has fired perfect. Using this technique I can perfect the ratio of raw:calcine for each Alberta Slip glaze I use. ![]() Roasting Alberta and Ravenscrag Slips at 1000F: Essential for good glazes Roasted Alberta Slip (right) and raw powder (left). These are thin-walled 5 inch cast bowls, each holds about 1 kg. I hold the kiln at 1000F for 30 minutes. Why do this? Because Alberta Slip is a clay, it shrinks on drying (if used raw the GA6-B and similar recipes will crack as they dry and then crawl during firing). Roasting eliminates that. Calcining to 1850F sinters some particles together (creating a gritty material) while roasting to 1000F produces a smooth, fluffy powder. Technically, Alberta Slip losses 3% of its weight on roasting so I should use 3% less than a recipe calls for. But I often just swap them gram-for-gram.
|